A.12.3. Chemglaze Z306 (also called Aeroglaze)

PRODUCT

Type

Flat back, Flexible, One-part Paint

Chemical Composition

Polyurethane

Manufacturer

Lord Corporation

          111 Lord Drive

          P.O.Box 8012

          Cary, NC 27512-8012, USA

Tel: +1 919 468 5979

Fax: 1 919 469 5777

Email:

www.lordcorp.com

Europe

Lord Corporation (Europe) Ltd.

          Barton Dock Rd.

          Stretford, Manchester M32 0ZH

          UK

Tel: +44 (0)161 865 8048

Fax:+ 44 (0)161 865 0096

Email:

www.lordcorp.com

EXPERIENCE & AVAILABILITY

Development Status

Commercial Product

Cost Range

Low

Lot Reproducibility

Good

Space Experience

Extensive

GENERAL PROPERTIES (Physical, Mechanical, Thermal, Electrical, Optical)

Nature

Typical Value

Remarks

Solid Content

26% to 29% (pbw)

Manufacturer’s Data

Viscosity

150 cps

Manufacturer’s Data

Solar Absorptance

0.95

ECSS-Q-70-09

Hemisperical Emittance

0.90

ECSS-Q-70-09

Shelf Life

1 Year

20°C

PROPERTIES RELEVANT TO SPACE USE (Effects of and/or on environment)

Nature

Typical Value

Type of Test

Flammability

Pass 24.5% O2. (on 1mm thick Aluminium foil).

NASA NHB 8060-1B

Outgassing

TML = 1.5%, RML = 0.6%, CVCM = 0.03%

ECSS-Q-70-02

UV/Particle Effects

Da = 0

7 Years/OTS spec.

Thermal Cycling

Pass

ECSS-Q-70-04

Offgassing/Toxicity

Pass

NASA NHB 8060-1A

SPECIAL RECOMMENDATIONS

·          Cuvertin 306 made by Henkel (Germany) generally shows higher TML/CVCM.

·          This paint (like most others) is not recommended for use in badly vented places where high electrical fields are present in the vicinity (corona risk).

·          Coating to be applied according to ECSS-Q-70-25 with use of Pyrolac P123 Primer.

·          Quality control tests by micro-VCM (ECSS-Q-70-02) are recommended.

·          Flammability test on 1mm thick Aluminium substrate in 24.5% O2. Material burns when applied to other substrates, e.g. Kapton. Configuration test mandatory.

·          This paint has been shown to contaminate space hardware returned from space. This is probably due to processing aids based on silicones.