Alloys with low resistance to stress-corrosion cracking The data given here is for information only. This table is divided according to the type of alloy. These types are : Steel alloys, Aluminium alloys, Copper alloys and Magnesium alloys Table III - Steel Alloys
Alloy | Condition | Carbon steel(1000 series) UTS Low alloy
steel(4130,4340 etc) UTS (E) D6AC, H-11 UTS 440C stainless steel 18 Ni Maraging steel, 200 grade 18 Ni Maraging steel, 250 grade 18 Ni Maraging steel, 300 grade 18 Ni Maraging steel, 350 grade AM 350 stainless steel AM 355 stainless steel Custom 455 stainless steel PH 15-7 Mo stainless steel 17-7 PH stainless steel CH900 (E)
Kovar | Above 140 kg/mm2 UTS Above 140 kg/mm2 UTS Above 148 kg/mm2 UTS All Aged at 900F Aged at 900F Aged at 900F Aged at 900F Below SCT 1000 Below SCT 1000 Below H1000 All except CH900 All except CH900 All |
Table III - Aluminium Alloys
Alloy, Wrought (1,2) | Condition | Alloy | Condition | 2011 2014 2017 2024 2024 Forgings 2024 Plate (E) 2618 7001 (E) 7020 7039 7075 7175 7079 7178 7475
(E) Al-Li 8090 (E) BS L93 (E) Russian Al-Li 1441 and 1460 | T3, T4 All All T3, T4 T6, T62, T8 T62 T3, T4 T6 Weldments All T6 T6 T6 T6 T6 All T6 All | 295.0 (195) B295.0 (B195) 520.0 (220) 707.0 (607,
tern-alloy 7) D712.0 (D612, 40E) |
T6 T6 T4 T6 As cast | 1) Mechanical stress relieved (TX5X or TX5XX) should be specified where possible.> 2) Sheet, unmachined extrusion and unmachined plate are the least susceptible forms.> (E) ESA classification - not in NASA MSFC-SPEC-522A.>
Table III - Copper Alloys
CDA no (1) | Condition (% cold rolled) (2) | 260
353 443 672 687 762 766 770 782 | 50 50 40 50, annealed 10, 40 A, 25, 50 38 38, 50, annealed 50 | 1) Copper Development Association alloy number
2) Rating based on listed conditions only
Table III - Magnesium alloys
Alloy | Condition |
Magnesium AZ61B Magnesium AZ80A WE54 ZCM711 | All All All All |
| |